(111) p-Si1e14, 50keV

Shots: 3a, 3b, 3c, 3d
3a, b shots had bad mask alignment; all others okay. All of them 2.5x2.5 mm. Shot with Harvard YAG, 1 shot at 0.7 J/cm2.

Sample 3a
6/7/2012           SEM/EBSD showing surface evidence of stacking faults, no obvious breakdown.
Au 4a Reflection.Sample.Raw.csv
6/8/2012           FIB-processed for TEM and imaged on JEOL 2100. Stacking faults throughout active layer observed.